An explanation and demo of atomic layer deposition (ALD) of copper metal on glass. Precursors are copper(I) chloride and hydrogen, processed in a hotwall tube quartz tube furnace.
10 torr operating pressure
500 sccm argon sweep/purge gas constantly flowing
75 sccm CuCl argon pulse gas (17 seconds including flow controller lag)
100 sccm H pulse gas (14 seconds including flow controller lag)
7 second purge time between pulses
100mm quartz tube furnace diameter
415*C deposition temperature
350*C CuCl evaporation temperature
Substrates are mostly borosilicate glass cleaned with RCA clean
The "good" samples shown in the video are about 750 cycles (about 9 hours
Main ref:
https://scihub.se/https://doi.org/10...
Also helpful:
https://scihub.se/https://doi.org/10...
https://scihub.se/10.1149/2.0261501jss
https://scihub.se/https://doi.org/10...
Alicat flow controller manuals (hard to find via website navigation):
https://documents.alicat.com/manuals/...
https://documents.alicat.com/manuals/...
https://documents.alicat.com/AlicatS...
RCA clean: https://en.wikipedia.org/wiki/RCA_clean
CuCl synthesis: http://wwwchem.uwimona.edu.jm/lab_man...
Support Applied Science on Patreon: / appliedscience